Tire R-rubber Encyclopedia

Four low cost tread reclaim rubber compound formulas

Create Date:2010-03-25 11:07:49Click volume:9720

The biggest advantage of reclaimed rubber is the low price of the product, which can greatly reduce the cost of raw materials for the production of rubber products. Among them, the price of tire reclaimed rubber is the lowest and the application is the most widely used. The reclaimed rubber with the highest amount of rubber in tire reclaimed rubber is used for mixing. Glue can significantly reduce costs. Xiao Bian today shares with you four of our engineers who have been working on the four low-cost compounding formulas for tread reclaimed rubber. We hope to help everyone.

Low Cost Tread Recycled Rubber Mix Formula 1: Natural Rubber, 100 Parts; Tread Reclaimed Rubber, 80 Parts; S, 2.6 Parts; Accelerator CZ, 1.3 Parts; Accelerator DM, 0.7 Parts; Zinc Oxide, 5.5 Parts Stearic acid, 2.5 parts; Antioxidant 4010, 1.0 part; Paraffin wax, 2.0 parts; Pine tar, 6.0 parts; High abrasion resistance N330, 50 parts; Light calcium carbonate, suitable amount; Solid Coumarone resin, appropriate amount.

Low Cost Tread Reclaimed Rubber Mix Formula 2: Natural Rubber, 100 Parts; Tread Reclaimed Rubber, 180 Parts; S, 4.0 Parts; Accelerator M, 0.8 Parts; Accelerator DM, 1.0 Part; Zinc Oxide, 7.5 Parts Stearic acid, 2.5 parts; Antioxidant 4010, 1.0 parts; Paraffin wax, 2.0 parts; Pine tar, 12.0 parts; High abrasion resistance N330, 30 parts; Light calcium carbonate, 65 parts; Solid Coomarone resin, appropriate amount.

Low Cost Tread Recycled Rubber Compound Formula 3: Natural Rubber, 100 Parts; Tread Reclaimed Rubber, 250 Parts; S, 5.0 Parts; Accelerator CZ, 1.2 Parts; Accelerator DM, 1.6 Parts; Zinc Oxide, 8.0 Parts Stearic acid, 4.5 parts; Antioxidant 4010, 1.0 part; Paraffin wax, 4.0 parts; Pine tar, 10.0 parts; High abrasion resistance N330, 25 parts; Light calcium carbonate, 150 parts; Solid Coomarone resin, moderate amount.

Low Cost Tread Reclaimed Rubber Compound Formula 4: Natural Rubber, 100 Parts; Tread Reclaimed Rubber, 265 Parts; S, 4.0 Parts; Accelerator M, 1.0 Parts; Accelerator DM, 1.3 Parts; Zinc Oxide, 8.5 Parts Stearic acid, 4.0 parts; Antioxidant 4010, 1.3 parts; Paraffin wax, 4.0 parts; Pine tar, 9.0 parts; High abrasion resistance N330, 35 parts; Light calcium carbonate, 70 parts; Solid Coomarone resin, appropriate amount.

Hebei Hongyun Reclaimed Rubber Factory has experienced rubber technical engineers who can design reclaimed rubber formulas, optimize formulas, and solve various problems encountered in the production of reclaimed rubber products.

Exclusive original article [commercial authorization] reprint, excerpt and excerpt in any form are prohibited without written authorization. Focus on Hongyun rubber: learn the process formula and raw material technology of producing rubber products from recycled rubber to help you reduce costs and increase profits